Fusion welding and heat calculations
Welding problems usually combine process identification with power, travel speed and melting volume. Track each efficiency from its own reference energy. The heat-affected zone belongs to the parent metal and does not melt.
7.1 Arc, gas and beam processes
Past papers · ME 2020–2026 (10 papers): 2 questions, 2 marks
| Process | Heat, electrode and protection | Selection point |
|---|---|---|
| Shielded metal arc (SMAW) | Consumable coated electrode; flux produces shielding and slag | Versatile manual work; stops for electrode changes and slag removal |
| Gas metal arc (GMAW: MIG/MAG) | Continuously fed consumable wire; external shielding gas | High deposition, automation; wire is compatible filler, not tungsten |
| Gas tungsten arc (GTAW/TIG) | Non-consumable tungsten, inert gas; separate filler optional | Controlled clean welds; generally lower deposition rate |
| Submerged arc (SAW) | Consumable wire under granular flux blanket | High deposition on suitable long seams; access/position restrictions |
| Flux-cored arc (FCAW) | Tubular consumable wire with flux; external gas may or may not be used | High deposition; slag and fumes depend on wire |
| Plasma arc | Constricted arc from electrode/nozzle arrangement | Concentrated heat, stable small arc |
| Oxy-fuel gas welding | Flame melts edges; separate filler optional | Portable equipment; broad heating and distortion |
| Laser beam | Focused light, often shielding gas; filler optional | Narrow, rapid seams; alignment/fit-up and reflectivity matter |
| Electron beam | Focused electrons, normally vacuum | Deep narrow welds; vacuum equipment and access constraints |
| Electroslag | Electrical resistance heating through molten slag after initiation | Heavy vertical sections; large heat input |
MIG uses inert shielding gas; MAG uses an active gas or mixture. In GMAW, the wire is both electrode and filler. Low-alloy-steel joints generally use compatible low-alloy-steel filler. In GTAW the tungsten carries current and is not intended to become filler. Laser welding is suitable for automotive tailor-welded blanks of different thickness because heat can be localised and seams automated.
An oxy-acetylene neutral flame has balanced primary oxygen/acetylene supply; an oxidising flame has excess oxygen, and a carburising/reducing flame has excess acetylene. Choose flame chemistry for the metal; neutral is the usual starting point for steel welding. Gas welding and gas cutting are distinct: cutting relies on an exothermic oxidation reaction and removal of oxide.
7.2 Arc power source and polarity
Past papers · ME 2020–2026 (10 papers): 1 question, 2 marks
Constant-current/drooping sources limit current changes with manual arc-length variations, as in SMAW and GTAW. A constant-voltage source with constant-speed wire feed supports arc-length self-regulation in GMAW: a shorter arc raises current and melt-off rate. In GTAW on steels, DC electrode negative (DCEN) avoids excessive tungsten heating; electrode-positive portions in AC help oxide cleaning for aluminium. Polarity effects depend on process; do not apply a fixed heat split to every arc.
7.3 Heat input, melting and filler feed
Past papers · ME 2020–2026 (10 papers): 2 questions, 4 marks
7.4 Resistance welding
Past papers · ME 2020–2026 (10 papers): 2 questions, 4 marks
Spot welding clamps overlapping sheets between water-cooled electrodes, passes current and forms a nugget at the sheet interface. The sequence is squeeze, weld-current interval, hold during solidification and release. Copper-alloy electrodes combine electrical/thermal conductivity with strength. Their contact resistance should be controlled so useful heating occurs at the joint, not mainly at the electrode faces.
Seam welding uses rotating wheel electrodes and overlapping welds. Projection welding concentrates current and force at designed projections. Resistance butt welding heats contacting ends; flash butt welding uses flashing followed by upsetting. Resistance spot welding is a fusion process despite the applied pressure.
7.5 Heat distribution and heat-affected zone
Past papers · ME 2020–2026 (10 papers): 2 questions, 2 marks
A fusion weld contains melted/re-solidified weld metal, an unmelted heat-affected zone (HAZ) and unaffected parent material. HAZ properties depend on peak temperature, time and cooling rate. Greater heat input per length generally broadens the HAZ in comparable material and geometry; concentrated beam welding commonly gives a narrow HAZ.
7.6 Weld defects and distortion
| Defect | Mechanism / control |
|---|---|
| Lack of fusion | Inadequate melting at a boundary; correct heat delivery, preparation and technique |
| Incomplete penetration | Root not fully fused; correct root gap, preparation and parameters |
| Porosity | Gas trapped during freezing; clean/dry surfaces and maintain shielding |
| Slag inclusion | Entrapped flux/slag; clean between passes and use suitable joint access |
| Undercut | Groove melted at toe and not filled; control current, speed and manipulation |
| Hot/solidification cracking | Weak segregated last-solidifying metal plus restraint; control composition and joint strain |
| Hydrogen-assisted cold cracking | Diffusible hydrogen, susceptible structure and tensile stress; low-hydrogen practice and appropriate preheat |
| Burn-through / excess penetration | Excess local heat for section and support |
| Distortion / residual stress | Nonuniform thermal expansion and contraction; balance sequence, restraint and heat input |
Preheating can reduce cooling rate and hydrogen-cracking risk but is not a universal remedy. Restraint can reduce movement while increasing residual stress. Back-step/skip sequences, balanced welds and presetting can control distortion. Weld inspection methods are in the Metrology and Inspection handbook.
Last-minute recall
- GMAW wire is consumable; GTAW tungsten is not intended as filler.
- DC power is voltage times current; a linear source has maximum power at half endpoints.
- Heat per length divides power by travel speed.
- Useful melting power equals melting energy density times melt volume rate.
- Separate filler/base fractions from thermal efficiencies.
- Spot-weld heating varies with current squared.
- The HAZ is heated parent metal that has not melted.
- A process name alone does not fix HAZ width or heat split.