Chapter 8

Solid-state welding, brazing and bonding

A joint need not melt the parent metals. Identify whether bonding comes from solid-state contact and deformation, molten filler wetting, or an adhesive layer. Surface preparation and loading direction are central to all three routes.

8.1 Solid-state welding processes

ProcessBonding mechanismTypical application or restriction
Friction weldingRelative rubbing produces heat; axial pressure/upset joins softened surfacesShafts, dissimilar combinations; rotary version needs suitable rotational geometry
Inertia friction weldingStored flywheel energy supplies rubbing workControlled rotational-energy input
Friction stir weldingRotating non-consumable tool heats and stirs material while traversing the jointAluminium panels and structures; backing/clamping and tool access needed
Diffusion bondingClean intimate contact under pressure at elevated temperature and timeHigh-integrity joints; surface condition and cycle time critical
Ultrasonic weldingHigh-frequency tangential vibration plus clamping disrupts interface filmsFoils, wires, thin metal assemblies; also polymers by a different thermal response
Cold pressure weldingLarge plastic deformation creates clean intimate metal contactDuctile materials and clean surfaces
Roll bondingRolling reduction joins suitably prepared contacting surfacesClad sheet and multilayers
Explosion weldingHigh-speed oblique collision with interfacial jettingLarge clad plates; specialised geometry and operation

Solid-state means no required bulk melting of the parent pieces. It does not mean no heating or no metallurgical change. Friction stir welding has a stirred region and thermomechanically affected material; insufficient stirring can leave tunnels or unbonded interfaces. No consumable filler is normally required in these standard solid-state routes.

8.2 Brazing and soldering

Past papers · ME 2020–2026 (10 papers): 1 question, 1 mark

Both processes melt a filler while keeping the parent material solid. Brazing filler has liquidus above 450∘450^\circC; soldering filler has liquidus at or below 450∘450^\circC. Both remain below the parent-metal solidus in the intended process. Clean wettable surfaces, appropriate clearance and flux or controlled atmosphere promote flow and bonding. Braze welding deposits filler in a joint without relying on capillary filling in the same way as ordinary brazing.

Brazing joins dissimilar materials and thin assemblies with less parent-metal heating than fusion welding. Applications include carbide tool tips and heat exchangers. Soldering serves electrical/electronic connections and low-temperature assemblies. Too large a joint gap weakens capillary filling; too small a real gap can impede flow and exclude filler through roughness/oxides. Flux removes or prevents oxides; it is not a substitute for degreasing and joint preparation.

8.3 Adhesive bonding

Adhesives transfer load through a cured or solidified layer. Thermosetting systems such as epoxies cure by chemical reaction; thermoplastic and hot-melt systems can soften with heat. Surface preparation, wetting, cure conditions and bond-line thickness control strength. Adhesion failure is at the interface; cohesive failure is within adhesive; the adherend itself can also fail.

Prefer load transfer in distributed shear/compression; peel and cleavage concentrate stress at an edge. Bonding can join metals to polymers/composites, spread load and seal simultaneously. Limitations include temperature, moisture/chemical ageing, creep, cure time and inspection/access requirements. Larger overlap does not increase real joint capacity indefinitely because shear stress is nonuniform. Joint preparation must suit the adherend rather than simply maximising roughness.

Last-minute recall

  • Solid-state joining can use considerable heat without bulk melting.
  • Friction stir uses a traversing non-consumable tool; friction welding rubs the pieces.
  • Diffusion bonding needs contact, temperature, pressure and time.
  • Brazing and soldering melt filler rather than parent metal.
  • The conventional filler-liquidus boundary is 450∘450^\circC.
  • Wetting and joint clearance control capillary filling.
  • Adhesive lap shear is only an average; peel and edge stresses can govern.

Revise offline: the whole Manufacturing Processes handbook as one PDF

51 pages · 2.0 MBFree to read online. Sign in to download the PDF.We save the handbook, version and request time in My downloads. Privacy policy

All chapters · Corrections