Chapter 3

Forming foundations

Forming changes shape through plastic flow while approximately preserving metal volume. Temperature, strain history, rate and friction set the required load. Use the flow law and analysis level given in the question.

3.1 Hot and cold working

Hot working occurs above the effective recrystallisation temperature for the material and processing time; cold working occurs below it. Room temperature is not the definition. Use absolute temperature when discussing a fraction of melting temperature.

FeatureCold workingHot working
StructureStrain hardening and texture accumulateRecovery/recrystallisation can reduce accumulated hardening
Force and ductilityHigher force; ductility consumedUsually lower force and larger workable strain
Accuracy and surfaceBetter dimensional control, no hot scaleThermal contraction, oxidation and scale complicate control
PropertiesStrength/hardness increase; residual stresses possibleGrain refinement and closure of suitable internal voids possible
Processing needIntermediate annealing may be neededTemperature and strain-rate control needed

Warm working lies between conventional cold and hot regimes. Forging grain flow can improve directional performance, but neither hot working nor cold working guarantees isotropic properties.

3.2 Volume, strain and reduction

Past papers · ME 2020–2026 (10 papers): 1 question, 2 marks

For successive reductions, Af/A0=∏j(1−rA,j)A_f/A_0=\prod_j(1-r_{A,j}) and true strains add. If width spreads during rolling, use w0h0L0=wfhfLfw_0h_0L_0=w_fh_fL_f. The thickness reduction alone no longer gives the length increase.

3.3 Flow stress, work and friction

Last-minute recall

  • Hot and cold refer to recrystallisation behaviour, not a fixed room-temperature boundary.
  • Metal volume is approximately conserved; porous powder compaction is an exception.
  • Successive fractional reductions multiply; logarithmic strains add.
  • Average flow stress is an integral divided by strain interval.
  • Forging peak load uses the stress at the current strain unless another model is given.
  • Coulomb coefficient and shear friction factor are not interchangeable.