Chapter 4

Bulk forming

Rolling, forging, extrusion and drawing use different tool contacts and force directions. Start with volume conservation, then select the appropriate pressure or work model. Geometry and friction limits must be checked before calculating a load.

4.1 Rolling bite and contact

Past papers · ME 2020–2026 (10 papers): 2 questions, 4 marks

Two rolls rotate in opposite senses to draw stock through a reducing gap. Two-high reversing mills reverse roll direction; three-high mills permit alternate passes without reversing rolls. Four-high and cluster mills back up smaller working rolls to reduce deflection. Smaller work-roll radius generally lowers contact length and separating force.

Small-angle rolling geometry and the change in friction direction around the neutral location.Small-angle rolling geometry and the change in friction direction around the neutral location.

4.2 Rolling load, torque and slip

Past papers · ME 2020–2026 (10 papers): 3 questions, 6 marks

Strip speed usually rises from entry to exit. Before the neutral location the roll drives the strip; after it the strip outruns the roll and friction on the strip reverses. Neutral means equal local tangential speeds, not zero pressure. Friction produces a pressure peak near this region; applied tensions reduce required rolling pressure.

Wavy edges indicate excess edge elongation relative to the centre; centre buckling indicates the opposite. Edge cracks reflect poor ductility or tensile stresses. Alligatoring splits the stock internally and is associated with nonuniform deformation and material defects. Roll bending and flattening change the gap/contact geometry; crown and backup rolls help control shape.

4.3 Forging and upsetting

Past papers · ME 2020–2026 (10 papers): 1 question, 1 mark

Open-die forging permits lateral spreading. Impression dies guide flow; flash in a narrow land increases resistance and encourages cavity filling. Flashless forging needs close control of billet volume. Hammers supply impact energy; presses apply load over a stroke. Die friction and surface chilling restrain the faces and cause barreling.

For a long strip compressed in plane strain, an elementary small-friction estimate is F≃Y′bℓ[1+μb/(2h)]F\simeq Y' b\ell[1+\mu b/(2h)], where bb is full width across the flow direction, ℓ\ell the long contact length, hh height and Y′=2σf/3Y'=2\sigma_f/\sqrt3 the von Mises plane-strain flow strength. This is a different geometry from cylindrical upsetting.

Common defects are laps from folded surfaces, unfilled corners from inadequate flow, die mismatch, scale pits and internal cracks. Lubrication lowers load and die wear; suitable preforms and fillets reduce severe local flow.

4.4 Extrusion

Past papers · ME 2020–2026 (10 papers): 1 question, 2 marks

Direct extrusion pushes a billet through a stationary die; billet–container sliding adds friction. In indirect extrusion, the die moves into the billet and extrudate passes through a hollow ram, substantially reducing that sliding. Hydrostatic extrusion transmits pressure through a fluid. Impact extrusion uses a rapid punch stroke, often for thin-walled containers.

Surface cracking can result from excessive temperature/speed; centre-burst or chevron cracks reflect unfavourable internal stress and die/reduction conditions. A pipe defect drags contaminated surface material towards the centre; discard the appropriate butt end. A very small die angle increases frictional path length; a large angle increases redundant deformation, so the actual optimum is not zero.

4.5 Wire and tube drawing

Past papers · ME 2020–2026 (10 papers): 1 question, 2 marks

Drawing pulls material through a reducing die. The exit section transmits the draw force and limits possible reduction. Lubrication reduces force; multiple passes and intermediate annealing permit large total reductions. Tube sinking uses no internal tool; a plug or mandrel gives better control of inside size and wall thickness.

For a constant-strength metal with Coulomb friction in a conical die, one elementary slab model gives σd=Y(1+Bd)[1−(Af/A0)Bd]/Bd\sigma_d=Y(1+B_d)[1-(A_f/A_0)^{B_d}]/B_d, where Bd=μcot⁡αdB_d=\mu\cot\alpha_d, μ\mu is the die–wire friction coefficient and αd\alpha_d is die semi-angle. It neglects redundant work and back tension; its Bd→0B_d\to0 limit is the ideal logarithmic result. Use a given draw model when the question specifies one.

Last-minute recall

  • Bite uses roll radius, not diameter; small-angle maximum draft is μ2R\mu^2R.
  • Arc length and projected contact length are different exact quantities.
  • Roll force uses the stated pressure model; torque must count powered rolls.
  • Friction reverses at the neutral location.
  • Upsetting increases area and usually flow stress, so the final load is often largest.
  • Direct extrusion has billet–container sliding; indirect extrusion largely removes it.
  • Extrusion force acts on entry area; draw force is draw stress times exit area.
  • The ideal 63.2%63.2\% draw reduction requires perfectly plastic, frictionless conditions.