Solidification, feeding and casting quality
Cooling controls whether the mould fills and whether the last liquid can feed contraction. Use heat-removing area rather than geometric surface area blindly. Gating carries the melt into the cavity; a riser supplies liquid during solidification.
2.1 Solidification and heat removal
Past papers · ME 2020–2026 (10 papers): 3 questions, 6 marks
Pure metals ideally freeze at one temperature; most alloys freeze between liquidus and solidus through a mushy zone. A eutectic composition is an important single-temperature exception. Near a cold mould wall, rapid nucleation gives a fine chill zone; directional growth can create columnar grains, followed by equiaxed grains where conditions allow. Inoculants promote nucleation.
| Shape and cooling assumption | Modulus |
|---|---|
| Cube, edge , six cooling faces | |
| Sphere, diameter | |
| Cylinder, diameter , height , both ends cooling | |
| Large plate, thickness , two broad faces cooling | Approximately ; edges neglected |
| Very long cylinder, diameter , ends neglected | Approximately |
2.2 Riser sizing and directional solidification
Past papers · ME 2020–2026 (10 papers): 2 questions, 3 marks
A riser must freeze after the region it feeds, supply enough metal and remain connected through an unfrozen feeding path. Larger modulus meets only the first requirement. Chills accelerate local freezing; insulating or exothermic sleeves delay riser freezing. A blind riser is enclosed in the mould; an open riser communicates with the atmosphere. A skim bob traps floating impurities.
For a cylindrical riser of radius and height , with its base joined to the casting, count only cooling surfaces. With side and top cooling, . With top insulated and base excluded, independent of height. Exclude the corresponding contact patch from casting cooling area when the question's geometry requires it.
2.3 Constant-head gating
Past papers · ME 2020–2026 (10 papers): 1 question, 2 marks
The pouring basin steadies entry; a tapered sprue carries metal down; the sprue well reduces abrupt turning effects; runners distribute metal; ingates connect runners to the cavity. Runner extensions and filters help trap inclusions. The choke controls flow. In a gating ratio, state the order: sprue-base area : total runner area : total ingate area.
A falling stream accelerates, so its required area decreases downwards. A straight oversized sprue can separate the stream from the wall and aspirate air. A full, appropriately tapered sprue reduces aspiration. Pressurised gating restricts downstream total area to keep passages full; unpressurised gating expands downstream area to reduce velocity. Numerical ratios depend on alloy and design.
2.4 Rising metal level during filling
Bottom gating into a tall cavity builds a pressure head that opposes incoming flow. Integrate continuity if the head changes appreciably; a single entry velocity is insufficient.
2.5 Fluidity and defect diagnosis
Past papers · ME 2020–2026 (10 papers): 1 question, 1 mark
Fluidity is the ability to fill a mould before freezing; it is not simply the reciprocal of viscosity. Superheat, freezing range, surface tension, oxide films, mould heat extraction and section thickness all matter. More superheat can improve filling but also increases oxidation, gas pickup and thermal demand.
| Observation | Likely mechanism | Useful correction |
|---|---|---|
| Misrun: incomplete shape | Melt freezes before complete filling | Improve flow path, pouring conditions and section design |
| Cold shut: seam where streams meet | Streams meet too cool or with oxide skins | Reduce interrupted filling, improve temperature and cleanliness |
| Shrinkage cavity / interdendritic porosity | Last liquid cannot feed contraction | Improve riser, feeding path and directional freezing |
| Blowholes / pinholes | Entrapped or evolved gas | Dry/vent mould and cores, degas melt as appropriate |
| Hot tear | Restrained contraction of weak partially solid metal | Improve collapsibility, fillets and section transitions |
| Cold crack | Stress after solidification | Reduce thermal gradients/restraint; suitable treatment |
| Sand inclusion / erosion | Mould material breaks away into melt | Strengthen mould and moderate impingement |
| Metal penetration | Metal enters sand pores | Suitable grain size, coating and compaction |
| Mismatch / core shift | Mould halves or core displaced | Locate and support accurately |
| Fins / flash | Metal enters parting gaps | Correct mould closing and clamping |
| Dross | Light oxide/impurity accumulation, often near top | Clean melt; skim, filter and avoid turbulent entrainment |
| Scab | Raised rough metal over a detached thin sand layer | Control sand expansion, bonding and ramming |
| Scar | Shallow surface blow/depression in foundry terminology | Control surface gas generation and mould condition |
2.6 Casting design decisions
Use gradual section changes, generous fillets and uniform walls where possible. An isolated heavy junction is a hot spot; feed or chill it. Place a riser so solidification proceeds towards it, not towards a closed remote pocket. Avoid abrupt impingement, excessive fall and unnecessary free surfaces in the gating path.
A high casting yield is desirable only after soundness is achieved. A smaller riser can increase numerical yield while making the part unusable. A chill changes local heat extraction, so comparing moduli with a single unchanged mould constant can become invalid.
Last-minute recall
- Chvorinov area means the assumed cooling area.
- Equal modulus gives equal freezing time only for equal thermal constants.
- The riser must satisfy thermal, volume and feeding-path requirements.
- Insulation changes the riser boundary condition.
- Constant-head fill time is volume divided by flow.
- Bottom-gated filling slows as back-pressure rises.
- Misrun is incomplete filling; cold shut is an unfused meeting of streams.
- Hot tears arise from restrained contraction during weak late solidification.