Chapter 4

Heat treatment and transformation control

Heat treatment changes microstructure through temperature, time and cooling path. Specify the starting state and desired product before choosing the treatment; hardness at a surface and hardenability through a section are different requirements.

4.1 Transformation products and time–temperature diagrams

Product from austeniteFormationTypical consequence at comparable carbon content
Coarse pearliteDiffusional transformation at relatively high subcritical temperatureCoarser spacing; lower hardness than fine pearlite
Fine pearliteGreater undercooling in pearlite rangeSmaller lamellar spacing; greater strength/hardness
BainiteTransformation below pearlite range and above martensitic rangeFine ferrite/carbide structure; useful strength–toughness balance
MartensiteRapid, diffusionless transformation on coolingCarbon-supersaturated structure; high hardness and internal stress
Tempered martensiteReheat quenched steel below A1A_1Carbon redistribution and carbide precipitation; better toughness

Steel martensite is commonly represented as body-centred tetragonal (BCT); tetragonality approaches BCC at very low carbon. Fresh martensite is not ferrite containing equilibrium cementite. Bainite is not simply fine lamellar pearlite. Hardness generally rises from coarse pearlite to fine pearlite to bainite to untempered martensite for comparable carbon, but exact ranking depends on treatment and composition.

A TTT diagram describes isothermal holding after rapidly bringing austenite to the chosen temperature. Start/finish curves indicate transformation progress; between them the structure is mixed. A CCT diagram describes continuous cooling and is the appropriate guide for continuous industrial cooling paths. Do not read a continuous path quantitatively from TTT curves as if it were an isothermal hold.

MsM_s and MfM_f denote martensite start and finish temperatures. Martensitic transformation is approximately athermal: below MsM_s, fraction depends primarily on temperature reached, rather than holding time. Retained austenite may remain when the final temperature is above MfM_f. Alloy and carbon content affect these temperatures and diffusional transformation kinetics. There is no universal one-second nose or universal critical cooling rate.

Schematic isothermal transformation map with separate start and finish curves. The curves are illustrative and must not be used for numerical heat-treatment design.Schematic isothermal transformation map with separate start and finish curves. The curves are illustrative and must not be used for numerical heat-treatment design.

4.2 Annealing, normalising and quench hardening

Past papers · ME 2020–2026 (10 papers): 1 question, 1 mark

TreatmentThermal routePrincipal objective/product
Full annealingAppropriate austenitising treatment, then slow furnace coolingSofter structure, improved ductility; typically coarse pearlite plus proeutectoid phase
NormalisingAustenitise, then still-air coolRefined transformation structure; usually harder than full annealing of the same plain-carbon steel
Process/recrystallisation annealingHeat cold-worked material sufficiently for recrystallisation; low-carbon steel generally below A1A_1Restore ductility without full austenitisation
Stress reliefSuitable subcritical treatmentReduce residual stresses with limited change to the intended structure
SpheroidisingProlonged holding near/below A1A_1, or suitable cycling around itRounded carbides in ferrite; improves machining/forming of high-carbon steel
HomogenisingHigh-temperature diffusion treatment within the solid rangeReduce composition segregation
Quench hardeningAustenitise, then cool fast enough to suppress unwanted diffusional productsForm martensite; normally followed by tempering

For hypoeutectoid steel, full austenitisation requires heating above A3A_3. Hypereutectoid tool steels are commonly hardened from between A1A_1 and AcmA_{cm} to retain some carbides and limit grain growth/retained austenite. Do not prescribe “above AcmA_{cm}” for every treatment. Soaking time must permit the required transformation without excessive grain growth.

Quench severity broadly increases from air to oil to water to brine under comparable conditions; agitation, bath temperature, vapour film and quenchant formulation can change the result. Faster cooling raises the risk of distortion and cracking. Low-carbon steel can form martensite but its attainable martensitic hardness is lower than that of higher-carbon steel.

4.3 Tempering, austempering and martempering

Tempering reheats quenched steel below A1A_1 to balance hardness, toughness and residual stress. For a plain-carbon steel, increasing tempering severity generally reduces hardness and increases ductility; some alloy tool steels show secondary hardening through alloy-carbide precipitation. Temper brittleness is a possible alloy/process-dependent exception to a monotonic toughness trend.

RouteHold and final coolingMain distinction
Quench and temperQuench to martensite, then reheat below A1A_1Final structure is tempered martensite
AustemperQuench to bainitic range, hold until bainitic transformation completes, then coolFinal intended structure is bainite
Martemper / marquenchQuench to near/just above MsM_s, hold to equalise section temperature without substantial diffusional transformation, then cool through martensitic rangeReduce thermal gradients; martensite still normally needs tempering

4.4 Hardenability and surface treatments

Past papers · ME 2020–2026 (10 papers): 2 questions, 2 marks

Hardness is a local indentation response. Hardenability is the ability to develop a hardened structure to depth under a given quench. In a Jominy end-quench test, one end of an austenitised standard specimen is water quenched; cooling rate generally decreases with distance from that end. A material retaining hardness farther from the end has greater hardenability. Maximum martensitic hardness depends strongly on carbon; alloying can increase hardenability without proportionally increasing maximum hardness.

ProcessWhat changes at the surface?Need for subsequent quenching
CarburisingCarbon diffuses into low-carbon steelNormally quench to harden the carbon-rich case
NitridingNitrogen forms hard nitrides in suitable steelsNo martensitic quench is required to produce the nitrided case
CarbonitridingCarbon and nitrogen diffuse into surfaceUsually followed by quenching
CyanidingCarbon/nitrogen introduced using a salt-bath routeUsually followed by quenching; distinct from gas carbonitriding
Flame hardeningLocal austenitisation, no intended composition changeLocal quenching; steel must have adequate carbon
Induction hardeningElectromagnetic heating produces local austenitisationLocal quenching; no intended carbon addition

Nitriding is generally a subcritical treatment with relatively low distortion and uses a lower temperature than conventional carburising, cyaniding or carbonitriding. Carburising provides a hard wear-resistant case and a tougher low-carbon core. Flame and induction hardening are transformation treatments; they do not turn a low-carbon surface into a high-carbon one. Induction frequency and heating time influence hardened depth; electromagnetic penetration depth is not identical to final case depth.

4.5 Recovery, recrystallisation and precipitation

During heating of cold-worked metal: recovery rearranges defects and reduces residual stress with limited loss of strength; recrystallisation creates new strain-free grains and sharply reduces hardness; subsequent grain growth increases grain size. Recrystallisation temperature is a time-dependent processing description, not a fixed phase boundary. More prior cold work generally lowers the temperature needed for recrystallisation within a stated time.

Age hardening requires appreciable solute solubility at the solution-treatment temperature and reduced equilibrium solubility at the ageing temperature. Sequence: solution treat → quench to retain a supersaturated solid solution → age to form strengthening precipitates. Natural ageing occurs near room temperature; artificial ageing uses a higher controlled temperature. Under-ageing has an insufficient precipitate distribution; peak ageing gives the selected strength maximum; over-ageing coarsens particles and often lowers strength. Selected Al–Cu, Al–Mg–Si and Al–Zn–Mg alloys are typical candidates; not all aluminium alloys are age hardenable.

4.6 Diffusion in heat treatment

Diffusion explains homogenisation, carburising and precipitation. Interstitial diffusion is often faster than substitutional diffusion; temperature and crystal structure matter. The equations below are simple one-dimensional models, not complete case-hardening specifications.

Last-minute recall

  • TTT means isothermal; CCT means continuous cooling.
  • Fresh martensite is supersaturated, not an equilibrium ferrite–cementite mixture.
  • Normalising generally cools faster than full annealing.
  • Tempering follows hardening; austempering produces bainite.
  • Martempering reduces temperature differences before martensite forms.
  • Jominy measures hardenability, not simply maximum hardness.
  • Carburising adds carbon; induction hardening does not.
  • Recovery, recrystallisation and grain growth are distinct stages.
  • Diffusion distances scale with the square root of time under the stated model.

Revise offline: the whole Engineering Materials handbook as one PDF

40 pages · 1.7 MBFree to read online. Sign in to download the PDF.We save the handbook, version and request time in My downloads. Privacy policy

All chapters · Corrections