Phase diagrams and iron–carbon equilibria
An equilibrium diagram gives phases and their compositions at a specified temperature, pressure and overall composition. It does not give transformation time or guarantee the microstructure after rapid cooling.
3.1 Components, phases and degrees of freedom
A component is an independent chemical constituent needed to specify composition. A phase is a physically and chemically homogeneous region. Multiple grains of the same crystal phase do not count as multiple phases. A microconstituent can contain several phases: pearlite contains ferrite and cementite.
3.2 Solid solutions and diagram boundaries
Past papers · ME 2020–2026 (10 papers): 2 questions, 2 marks
A substitutional solid solution replaces host atoms; an interstitial solution places small atoms in interstices (carbon in iron). Extensive substitutional solubility is favoured by similar atomic radii (roughly within 15%), same crystal structure, similar electronegativity and compatible valency. These Hume–Rothery guidelines favour solubility; they do not prove complete miscibility.
| Boundary or region | How to read it |
|---|---|
| Liquidus | Above it the alloy is fully liquid |
| Solidus | Below it the alloy is fully solid |
| Solvus | Composition limit between a solid solution and two solid phases |
| Two-phase field | Draw a horizontal tie line; endpoints give phase compositions |
| Isomorphous system | Complete solid solubility; typical example Cu–Ni |
| Eutectic system | A liquid can transform to two solids at one invariant temperature |
In an isomorphous solidification range, the first solid and remaining liquid generally differ in composition. Limited solid diffusion causes coring (composition gradients within grains); a sufficiently long homogenising treatment can reduce it. A miscibility gap is an equilibrium two-phase composition range, not another name for coring.
3.3 Lever rule and fraction conversion
A schematic eutectic diagram showing the distinction between phase composition and phase amount. Coordinates are illustrative, not alloy data.
3.4 Invariant reactions and cooling paths
| Reaction on cooling | Reactants → products | Recognition |
|---|---|---|
| Eutectic | One liquid produces two solids | |
| Eutectoid | One solid produces two other solids | |
| Peritectic | Liquid and solid produce a new solid | |
| Peritectoid | Two solids produce a new solid | |
| Monotectic | One liquid produces another liquid and a solid |
denotes liquid; Greek letters denote distinct solid phases. Reactions reverse on heating. At fixed pressure each is invariant in a binary system with three coexisting phases. Eutectic alloys solidify at a single temperature under equilibrium; a general off-eutectic alloy solidifies over a range. A cooling-curve arrest indicates latent heat release, not elapsed transformation time read from an equilibrium diagram.
For a hypoeutectic composition, primary forms before the eutectic reaction; the remaining liquid becomes the eutectic microconstituent. The eutectic fraction equals the liquid fraction just above the reaction. For a hypereutectic composition, primary forms first. Below the reaction, total phase fractions and fractions of primary/eutectic microconstituents are different questions.
3.5 Iron–cementite reference values
Past papers · ME 2020–2026 (10 papers): 1 question, 1 mark
The conventional Fe–FeC diagram is metastable with respect to graphite. It is the standard reference for ordinary steel transformations. The stable Fe–graphite system matters for graphitic cast irons; cooling rate and silicon influence whether carbon appears as graphite or carbide.
| Phase/constituent | Structure or constituents | Key property |
|---|---|---|
| ferrite | BCC iron solid solution | Soft, ductile; very low carbon solubility |
| austenite | FCC iron solid solution | Higher carbon solubility; parent for steel heat treatment |
| ferrite | High-temperature BCC iron solid solution | Distinct high-temperature stability field |
| Cementite, FeC | Iron carbide; approximately 6.67 wt% C | Hard and brittle |
| Pearlite | Lamellar ferrite + cementite | Eutectoid microconstituent, not a phase |
| Ledeburite | Austenite + cementite at formation | Eutectic constituent; austenite subsequently transforms |
| Landmark | Temperature, approximately | Compositions, approximately (wt% C) |
|---|---|---|
| Eutectoid | C | |
| Eutectic | C | |
| Peritectic | C | |
| Maximum C in ferrite | At eutectoid | About 0.022 |
| Maximum C in austenite | At eutectic | About 2.14 |
The lower critical boundary is the eutectoid temperature; separates from ; separates from . denotes the magnetic transition, not a structural phase boundary. Heating () and cooling () critical temperatures can differ from equilibrium values because of kinetics.
3.6 Steel phase and microconstituent fractions
Past papers · ME 2020–2026 (10 papers): 2 questions, 4 marks
Take as eutectoid carbon content, ferrite carbon content at that temperature, and cementite carbon content, all in wt%. Write for cementite only in these fraction equations. Slow cooling and complete eutectoid transformation are assumed.
Pearlite, total cementite and proeutectoid cementite are different fractions. Curves use the stated 0.76, 0.022 and 6.67 wt% reference values.
Last-minute recall
- At fixed pressure, a binary three-phase equilibrium is invariant.
- Tie-line endpoints give compositions; opposite arms give amounts.
- Weight-percent axes produce mass fractions.
- Pearlite and ledeburite are microconstituents containing two phases.
- Hypoeutectoid steel gives proeutectoid ferrite; hypereutectoid gives proeutectoid cementite.
- Pearlite fraction is inherited from austenite just above .
- Total cementite includes cementite inside pearlite.
- The equilibrium diagram does not predict martensite fractions or cooling rates.