Metals and alloys: properties to applications
Choose a material by the required combination of strength, toughness, wear, corrosion resistance, temperature capability, density and manufacturability. Family names alone do not specify numerical strength; grade and heat treatment matter.
5.1 Plain-carbon and alloy steels
| Family | Main tendency | Common application |
|---|---|---|
| Low-carbon steel | Good ductility/formability and weldability; limited through-hardening hardness | Sheets, welded structures, carburised gears |
| Medium-carbon steel | Greater strength and heat-treatment response; less easy forming/welding | Shafts, axles, crankshafts |
| High-carbon steel | High attainable hardness and wear resistance; reduced weldability/ductility | Springs, wire, simple cutting/wear tools |
| Low-alloy engineering steel | Alloy-controlled hardenability and strength–toughness balance | Highly loaded gears, shafts, fasteners |
| Tool/high-speed steel | Carbides support wear resistance; suitable alloying retains hot hardness | Dies, drills, milling cutters |
| Maraging steel | Age-strengthened low-carbon martensitic matrix | High-strength tooling and demanding structural parts |
Carbon categories are approximate; commonly low is up to about 0.3 wt%, medium about 0.3–0.6%, and high above about 0.6%. These are engineering labels, not phase boundaries. Increasing carbon in comparable slowly cooled plain-carbon steels generally increases pearlite/carbide fraction, strength and hardness while reducing ductility and weldability.
| Addition | Useful effect; avoid treating it as universal |
|---|---|
| Mn | Deoxidiser; binds sulphur as MnS and improves hardenability |
| Si | Deoxidiser; electrical steels use its effect on resistivity; promotes graphitisation in cast iron |
| Cr | Hardenability/carbides; adequate dissolved chromium supports passivation |
| Ni | Austenite stabilisation; can improve toughness |
| Mo | Hardenability and elevated-temperature performance; carbide effects |
| V, Nb, Ti | Carbide/nitride precipitation and grain-size control |
| W | Alloy carbides and hot hardness in tool steels |
| S, P | Often restricted for toughness; sulphur may be deliberately used for free machining |
Hadfield steel is a high-manganese austenitic wear-resistant steel that work hardens under impact, useful in crusher parts. Manganese is Mn; magnesium Mg is a different element. Killed steel is strongly deoxidised before solidification; the term does not mean quench hardened.
5.2 Stainless steels and hot-service alloys
Stainless steels rely on a chromium-rich passive surface film; corrosion resistance is environment dependent. A common austenitic composition is described as 18–8 (nominal chromium–nickel percentages), but this is not the definition of every stainless steel.
| Stainless family | Structure/response | Typical use |
|---|---|---|
| Austenitic | FCC; generally ductile and nonmagnetic when solution annealed; not hardened by ordinary quench-and-temper treatment | Food/chemical equipment, cryogenic components |
| Ferritic | BCC; magnetic; not conventionally martensitically hardened | Exhaust systems, sheet applications |
| Martensitic | Quench hardenable; magnetic; hardness–corrosion compromise | Cutlery, blades, some turbine parts |
| Duplex | Ferrite + austenite; useful strength and corrosion resistance | Process equipment, marine service in suitable grades |
| Precipitation hardening | Strength developed by ageing an appropriate treated structure | High-strength corrosion-resistant components |
Sensitisation can occur when chromium carbides form at grain boundaries and deplete adjacent regions of chromium; it can promote intergranular corrosion. Low-carbon or suitably stabilised grades and suitable thermal processing reduce this risk. Cold working can make some initially austenitic grades partly magnetic.
Ni-, Co- and Fe-based superalloys combine high-temperature strength with oxidation/corrosion resistance. Selected Ni-based turbine-blade alloys use precipitation strengthening and directional solidification or single crystals to improve creep performance. A superalloy need not be single crystalline; a whisker is a slender single-crystal reinforcement, not a thin sheet of superalloy.
5.3 Cast irons
Past papers · ME 2020–2026 (10 papers): 1 question, 1 mark
Graphite shape is central to cast-iron behaviour. Silicon and slower cooling favour graphite; rapid cooling and carbide-promoting conditions favour white iron. Matrix composition and heat treatment further change properties.
| Type | Carbon morphology / production distinction | Properties and use |
|---|---|---|
| Grey iron | Graphite flakes in a metallic matrix | Excellent damping and machinability; low tensile ductility; machine beds, housings, brake discs |
| White iron | Carbon largely in carbides rather than free graphite | Very hard, brittle and wear resistant; wear liners and rolls |
| Ductile / nodular / SG iron | Spheroidal graphite, commonly from melt treatment with Mg | Better tensile ductility/toughness than flake graphite iron; pipes, crankshafts, gears |
| Malleable iron | Heat treatment of suitable white-iron castings produces temper carbon aggregates | Tougher than white iron; fittings and small cast parts |
| Chilled iron | Rapid local cooling creates a white hard surface with a different core | Wear-resistant rolls and selected contact surfaces |
| Compacted graphite iron | Short, rounded interconnected graphite rather than long flakes | Intermediate mechanical/thermal behaviour; engine blocks |
5.4 Non-ferrous engineering alloys
| Material/family | Useful property combination | Common application / limitation |
|---|---|---|
| Aluminium alloys | Low density; good conductivity and corrosion resistance; selected alloys age harden | Aircraft/transport structures, heat exchangers; modulus lower than steel |
| Al–Si casting alloys | Good castability and useful wear/corrosion behaviour | Housings, engine castings; do not infer age hardenability from Si alone |
| Copper | Excellent electrical/thermal conductivity and ductility | Conductors, heat exchangers |
| Brass (Cu–Zn) | Formability, machinability in suitable grades | Fittings, tubes, hardware |
| Tin bronze (Cu–Sn) | Wear/corrosion resistance; suitable bearing behaviour | Bushes, bearings, gears; other named bronzes need not contain Sn |
| Cu–Ni | Corrosion resistance in suitable marine environments | Condenser and marine heat-exchanger tubes |
| Magnesium alloys | Very low density; useful specific properties | Lightweight housings; corrosion and temperature limits need attention |
| Titanium alloys | High specific strength and corrosion resistance | Aerospace and chemical equipment; cost and processing constraints |
| Nickel alloys | Corrosion and/or high-temperature performance | Chemical plant, hot-section components |
| Zinc alloys | Good pressure die-casting capability | Small intricate housings and fittings |
“Specific strength” compares strength divided by density; “specific stiffness” compares modulus divided by density. Always compare the relevant strength mode and service temperature. Wear resistance, corrosion resistance and thermal conductivity do not necessarily improve together.
Last-minute recall
- Carbon classification and eutectoid classification are different.
- Low carbon favours forming/welding; higher carbon permits greater martensitic hardness.
- Mn and Mg have different functions and cannot be interchanged.
- Chromium passivation depends on the local material state and environment.
- Austenitic stainless steel is not ordinarily quench hardened.
- Flake graphite aids damping but is unfavourable for tensile ductility.
- Nodular iron is melt treated; malleable iron is heat treated from white iron.
- Brass is Cu–Zn; tin bronze is Cu–Sn.