Separate a test result from a design estimate. Specimen geometry, curing, moisture at test, age and load duration affect measured properties even when the mix is unchanged.

5.1 Strength tests

Past papers · CE 2020–2026 (14 papers): 2 questions, 2 marks

Compression is carried much better than tension. Concrete shows a nonlinear compression curve with progressive microcracking; tension failure is comparatively brittle. Cube strength is generally higher than cylinder strength because specimen proportions and end restraint differ. A fixed conversion factor is only an approximation for specified conditions.

IS 516 (Part 1/Sec 1):2021 covers compressive, flexural and split tensile testing. Older questions may explicitly cite IS 5816:1999 for splitting; the cylindrical splitting expression above is unchanged. The question's stated method governs.

Air-dried and saturated specimens do not necessarily give equal strength; dry specimens often test stronger than comparable saturated specimens. Poor curing reduces hydration; temperature history and test loading rate also matter. A rebound hammer measures surface response and ultrasonic pulse velocity measures wave transit; neither gives a universal strength conversion without calibration.

5.2 Elastic and tensile estimates

Tangent modulus is the local slope of a stress–strain curve; secant modulus joins the origin to a specified point. Longer loading duration generally gives greater strain and a smaller apparent secant modulus. Aggregate stiffness significantly influences concrete modulus.

5.3 Creep, shrinkage and thermal strain

Past papers · CE 2020–2026 (14 papers): 2 questions, 2 marks

Creep is additional deformation under sustained stress. Shrinkage occurs without imposed stress: plastic shrinkage occurs before hardening; drying shrinkage accompanies moisture loss; autogenous shrinkage is associated with internal water consumption and self-desiccation. Restrained shrinkage can create tensile stress and cracks.

Loading ageIS 456:2000 approximate ultimate θc\theta_c, absent specific test data
7 days2.2
28 days1.6
1 year1.1

Younger loading, longer duration, lower humidity, more paste and smaller effective member size generally increase creep; constituent and curing effects also matter. Ultimate creep strain excludes the immediate elastic strain. Under fixed strain, stress can relax instead.

5.4 Curing and removal of support

Past papers · CE 2020–2026 (14 papers): 2 questions, 2 marks

Curing maintains moisture and temperature for hydration and strength development. Ponding, wet coverings, continuous spraying and approved membranes are different means to that end. Poor curing particularly harms the near-surface zone, even when an interior cube appears satisfactory.

SituationIS 456:2000 moist-curing guidance
OPC concreteAt least 7 days
Concrete with blended cement or mineral admixtureAt least 10 days
Dry and hot weatherAt least 10 days; for blends/mineral admixtures, extension to 14 days is recommended

Formwork must retain shape without losing mortar and must support construction loads. Removal depends on attained strength and the temporary structural system. Under IS 456:2000, the strength guiding removal is at least twice the stress that will occur at that stage, assessed for comparable curing conditions.

Formwork operationNormal indicative minimum, OPC, adequate curing, ambient temperature not below 15°C
Vertical sides of columns, walls and beams16–24 h
Slab soffit forms, props immediately refixed3 days
Beam soffit forms, props immediately refixed7 days
Slab props: span up to 4.5 m / over 4.5 m7 / 14 days
Beam/arch props: span up to 6 m / over 6 m14 / 21 days

For a cantilever, remove props progressively from the free end towards the fixed support, subject to the approved sequence and adequate attained strength. This avoids turning the member temporarily into an unintended supported-span system. For simply supported spans, removal generally progresses from the centre towards the supports. A figure's labels must be located before choosing a labelled sequence.

Last-minute recall

  • A cube strength is maximum load divided by loaded area.
  • Splitting strength uses 2F/(πLD)2F/(\pi LD).
  • Flexural test coefficients depend on loading arrangement and fracture location.
  • 5000fck5000\sqrt{f_{ck}} and 0.7fck0.7\sqrt{f_{ck}} require MPa.
  • Creep is load-dependent; shrinkage occurs without imposed load.
  • Creep coefficient multiplies immediate elastic strain to give additional creep strain.
  • Free shrinkage is negative under a tension-positive convention.
  • Mineral additions/blended cements usually need a longer moist-curing period.
  • Cantilever props are removed from the free end towards the fixed end.