Chapter 4

Concrete mix design

A mix must satisfy strength, workability and durability together. Select the free water ratio, calculate absolute volumes and then verify by trials; a nominal proportion alone cannot guarantee a concrete grade.

4.1 Characteristic and target strength

Past papers · CE 2020–2026 (14 papers): 2 questions, 2 marks

fckf_{ck} is the characteristic 28-day compressive strength of a 150 mm concrete cube: no more than 5% of the strength population is expected to fall below it. M30 denotes fck=30f_{ck}=30 MPa. This statistical definition is different from code acceptance rules for a batch of test results.

GradeAssumed sfs_f, MPa, good site controlXX, MPa, IS 10262:2019
M10, M153.55.0
M20, M254.05.5
M30 to M605.06.5
M65 to M806.08.0

Use established test data in preference to assumed variability when adequate. For fair rather than good control, the listed assumed standard deviation is increased by 1 MPa. The normal model is a statistical approximation; the code margin is a separate prescription.

4.2 Water ratio and durability limits

Past papers · CE 2020–2026 (14 papers): 1 question, 1 mark

Free water excludes water absorbed within SSD aggregate. Total binder includes cement and the specified cementitious additions. Use the ratio named in the problem: water–cement ratio and water–binder ratio differ when cement replacement is present.

At fixed constituents, compaction, age and curing, increasing free water ratio generally lowers strength and increases permeability. At fixed cement content it generally increases workability. Very low water ratio without suitable admixture/compaction can instead produce voided concrete.

IS 456:2000 durability limits below apply to normal-weight aggregate of 20 mm nominal maximum size. Entries are minimum cement content in kg/m³ / maximum free water–cement ratio / minimum grade.

ExposurePlain concreteReinforced concrete
Mild220 / 0.60 / not specified in this table300 / 0.55 / M20
Moderate240 / 0.60 / M15300 / 0.50 / M25
Severe250 / 0.50 / M20320 / 0.45 / M30
Very severe260 / 0.45 / M20340 / 0.45 / M35
Extreme280 / 0.40 / M25360 / 0.40 / M40

For 10 mm aggregate, add 40 kg/m³ to the table's minimum cement content; for 40 mm, subtract 30 kg/m³. Ordinary cement content above 450 kg/m³ needs special consideration of cracking and other risks under IS 456:2000; distinguish cement from permitted mineral additions. Contributions of additions to the durability binder requirement require the applicable code conditions. Select the more restrictive strength/durability water ratio and satisfy the minimum grade independently.

4.3 Absolute-volume proportioning

Choose aggregate size, grading, desired slump, air and admixture before solving the volume balance. The normal-concrete starting estimates below are from IS 10262:2019; they require trial adjustment.

Maximum nominal size, mmWater for angular aggregate, 50 mm slump, kg/m³Approximate entrapped air, % of concrete volumeCoarse fraction, Zone I sandZone IIZone IIIZone IV
102081.50.480.500.520.54
201861.00.600.620.640.66
401650.80.690.710.720.73

Coarse fractions are fractions of total aggregate absolute volume at water ratio 0.50, for SSD crushed aggregate. They are not fractions of total concrete volume. Zone IV sand needs suitability trials for reinforced concrete. The table is a normal-concrete starting point; do not use it unchanged for high-strength, self-compacting or mass concrete.

4.4 Trial sequence, yield and special mixes

Check slump, cohesion, bleeding, density and strength in trial batches. If workability is changed by adjusting water, recalculate binder to preserve the selected ratio. IS 10262:2019 uses further trials around the selected water ratio, approximately ±10%, to establish the strength–ratio relation. Correct to actual field moisture and production conditions.

Mix typeAdditional concern within the same strength–workability–durability framework
High-strength concreteLow water–binder ratio, compatible high-range water reducer, strong aggregate and careful curing; IS 10262:2019 treats M65 and above separately
Self-compacting concreteFilling ability, passing ability and segregation resistance together; high flow alone is insufficient
Mass concreteTemperature rise and gradients, placement sequence and low-heat binder strategy
Air-entrained concreteControlled air for exposure resistance; account for its volume and strength effect
Lightweight concreteAggregate absorption and density require specific data; normal-weight empirical constants may not apply

Nominal mixes may be permitted for specified lower grades under the applicable code; design mixes use performance-based trial proportions. Do not equate a loose-volume recipe with a guaranteed characteristic strength.

Last-minute recall

  • Characteristic strength is a lower-tail value, not the mean.
  • IS 10262:2019 requires the larger of two target-strength expressions.
  • Cement and total binder are different denominators in blended mixes.
  • Lower water ratio helps only if concrete is properly compacted and cured.
  • Absolute volumes include air and chemical admixture.
  • Coarse-aggregate fraction refers to aggregate volume, not concrete volume.
  • Moisture correction follows SSD proportioning; it does not change the required free-water ratio.
  • Trial strength and workability are essential checks on calculated proportions.

Revise offline: the whole Construction Materials and Management handbook as one PDF

51 pages · 2.2 MBFree to read online. Sign in to download the PDF.We save the handbook, version and request time in My downloads. Privacy policy