Concrete constituents and fresh behaviour
Aggregates occupy most of the volume; water controls both hydration and placement. Track the moisture condition and the measurement basis before combining masses or volumes.
3.1 Aggregate grading and fineness modulus
Past papers · CE 2020–2026 (14 papers): 1 question, 1 mark
Coarse aggregate is predominantly retained on the 4.75 mm sieve; fine aggregate predominantly passes it. Well-graded particles reduce voids and paste demand. Angular, rough particles generally need more paste/water for the same workability than rounded, smooth particles. Flaky and elongated particles can hinder compaction and packing.
For sand, the larger-sieve cumulative retentions may be zero. Include the 150 µm cumulative retention even when no particles are retained individually on that sieve. Exclude the pan. Higher indicates coarser aggregate, but identical does not imply identical grading. Grading zones I to IV progress broadly from coarse to fine sand; alone does not establish compliance with a zone.
3.2 Aggregate moisture, absorption and bulking
Oven dry (OD) aggregate has empty accessible pores; saturated surface dry (SSD) aggregate has saturated pores but no surface film. Air-dry aggregate lies between them. Wet aggregate has surface water that contributes to mixing water.
Specific gravity is particle density divided by water density, not loose bulk density divided by water density. Use an SSD specific gravity with SSD aggregate mass in absolute-volume mix calculations. Aggregate bulk unit mass includes interparticle voids.
3.3 Mixing water and constituent quality
Past papers · CE 2020–2026 (14 papers): 1 question, 1 mark
IS 456:2000 specifies pH not less than 6 for mixing water. Potable water is generally suitable, but the water must be free of harmful amounts of oils, acids, alkalis, salts, sugars and organic material. Sea water is unsuitable for routine reinforced-concrete mixing/curing because salts can affect durability and corrosion.
| Permissible solid in mixing water | IS 456:2000 maximum, mg/L |
|---|---|
| Organic solids | 200 |
| Inorganic solids | 3000 |
| Sulphates, expressed as | 400 |
| Chlorides, as Cl, without embedded steel | 2000 |
| Chlorides, as Cl, reinforced concrete | 500 |
| Suspended matter | 2000 |
These are limits for water, not allowable total chloride contents of concrete. Under the code's comparative strength check for doubtful water, the average 28-day cube strength is at least 90% of the corresponding distilled-water control. Initial set must be at least 30 min and within 30 min of the control. Low pH is not the only possible water-quality defect.
Aggregate should be durable and clean. Clay coatings impair bond; salts and organic impurities can disturb setting and durability. Alkali–silica reaction needs reactive silica, sufficient alkali and moisture; control the constituent combination rather than assuming every silica-bearing aggregate reacts.
3.4 Workability, segregation and bleeding
Workability describes the ease of mixing, transporting, placing and compacting concrete without losing uniformity. It is not the same as water content. Cohesion and the available compaction method matter along with flow.
| Test | Result | Most useful interpretation |
|---|---|---|
| Slump | Vertical subsidence in mm | Common field consistency check for plastic concrete |
| Compacting factor | Mass/density ratio | More sensitive for relatively low-workability mixes |
| Vee-Bee | Remoulding time in seconds | Stiff mixes; shorter time means greater workability |
| Flow/slump flow | Spread under the specified method | Flowable mixtures; report the test and unit |
A slump cone is 300 mm high, 200 mm at the base and 100 mm at the top. True slump indicates coherent settlement; shear slump calls for reassessment/repetition; complete collapse does not supply a useful ordinary slump value. Slump is neither a direct strength test nor a complete measure of workability.
Segregation is separation of constituents; excessive fall, unsuitable grading, over-wet mixes or excessive vibration can cause it. Bleeding is upward migration of water as solids settle. Bleed channels and water pockets below aggregate/reinforcement can impair bond; finishing before bleed water dissipates can weaken the surface. Fine materials and proper proportioning improve cohesion, but excessive fines increase water demand.
Last-minute recall
- Fineness modulus adds cumulative retained percentages, including the fine end of the standard series.
- is dimensionless; ten-percent-fines value is a force.
- SSD aggregate contributes neither surface water nor an absorption deficit.
- Moisture and absorption percentages must have the same mass basis.
- Bulking changes loose volume, not the mass of sand solids.
- Mixing-water pH must be at least 6 under IS 456:2000.
- Slump, compacting factor and Vee-Bee time have different units and useful ranges.
- Bleeding is water movement; segregation is broader constituent separation.