Chapter 2

Cement chemistry and admixtures

Cement reacts with water; it does not harden merely by drying. Identify the clinker phase, the hydration product and the effect on fresh or hardened concrete separately.

2.1 Oxides and clinker compounds

Past papers · CE 2020–2026 (14 papers): 2 questions, 2 marks

In cement chemistry notation, C=CaOC=\mathrm{CaO}, S=SiO2S=\mathrm{SiO_2}, A=Al2O3A=\mathrm{Al_2O_3}, F=Fe2O3F=\mathrm{Fe_2O_3} and H=H2OH=\mathrm{H_2O}. Here letters represent oxide units, not cost, area, force or time. Limestone supplies much of the calcium; clay/shale supplies silica and alumina. Burning produces clinker; grinding with controlled calcium sulphate regulates setting.

PhaseChemical shorthandMain revision association
Tricalcium silicate (alite)C3SC_3SFaster hydration; major early-age strength contribution; more heat than C2SC_2S
Dicalcium silicate (belite)C2SC_2SSlower hydration; later-age strength; lowest heat among these four principal phases
Tricalcium aluminateC3AC_3AVery rapid reaction without sulphate control; flash-set risk; highest heat among these phases
Tetracalcium aluminoferriteC4AFC_4AFFerrite phase; contributes colour and acts in clinker formation; smaller strength contribution

For the usual comparative question, heat of complete hydration follows C3A>C3S>C4AF>C2SC_3A>C_3S>C_4AF>C_2S approximately; measured heat also depends on age and reaction extent. Increasing the C2SC_2S share at the expense of faster, hotter phases reduces early heat evolution. Avoid memorising a fixed heat value for all cements.

Excess free lime and periclase can cause delayed expansion; they are different from calcium already bound in stable silicates. Higher fineness increases reactive surface and early reaction rate but can increase water demand and early heat.

2.2 Hydration, setting and microstructure

Past papers · CE 2020–2026 (14 papers): 1 question, 1 mark

C–S–H binds the solid skeleton and supplies most strength. Calcium hydroxide helps maintain alkalinity but is more vulnerable to leaching and chemical attack. The aluminate reaction with gypsum initially forms ettringite; later sulphate depletion can permit monosulphate formation. Proper early ettringite formation is normal. Expansive formation in an already rigid microstructure is a different situation.

FeatureMeaning and consequence
Gel poresVery small pores within hydration products; distinguish from larger capillaries
Capillary poresSpace not filled by solid products; connected pores strongly influence transport and permeability
Unhydrated grainsRemain when reaction is incomplete; not automatically evidence of failed concrete
Interfacial transition zone (ITZ)Paste near aggregate commonly has greater local porosity and microcracking than bulk paste
Higher degree of hydrationMore products and, generally, less connected capillary space
Higher initial water–cement ratioMore space to be filled; generally greater remaining capillary porosity at equal hydration

Hydration heat rate typically shows an initial reaction, an induction period, acceleration, deceleration and a slow continuing reaction. Setting is loss of plasticity; hardening is strength gain. Initial set does not mean adequate structural strength.

2.3 Cement selection and routine tests

IS 269:2015 consolidates ordinary Portland cement grades 33, 43 and 53. A cement grade is based on standard mortar strength, not on the strength of concrete made with that cement. PPC uses a pozzolanic component; Portland slag cement uses granulated blast-furnace slag. Low-heat cement is useful where temperature rise matters; sulphate-resisting cement limits vulnerable aluminate content. Rapid-hardening cement gives early strength; it need not be a quick-setting cement.

Test/propertyWhat to retainOrdinary OPC reference
Standard consistencyVicat plunger endpoint determines water needed for a specified paste consistencyIt is a measured result, not a universal water–cement ratio
Initial settingTime from adding water until the specified needle endpointAt least 30 min
Final settingTime to the specified final-set endpointAt most 600 min
FinenessBlaine specific surface or specified sieve methodBlaine minimum 225 m²/kg for ordinary OPC
SoundnessExcessive expansion tendencyLe Chatelier maximum 10 mm; autoclave maximum 0.8%
Standard mortar strengthSpecified cement–standard-sand specimen and curing28-day minimum 33, 43 or 53 MPa for the corresponding OPC grade

The test limits above refer to IS 269:2015 ordinary grades, not every special cement. A Le Chatelier test is chiefly sensitive to free-lime expansion; autoclave testing is also sensitive to magnesia-related unsoundness. Cement specific gravity near 3.15 is a usual OPC calculation assumption, not a substitute for measured specific gravity of a blended binder.

2.4 Chemical admixtures

Chemical admixtures alter fresh behaviour or reaction at comparatively small dosages. Select dosage through trials with the actual cement and temperature. A beneficial change in one property can adversely affect another.

TypeIntended actionCommon trap
Water reducer/plasticiserDisperses particles; same workability with less water, or higher workability at the same waterStrength rises through reduced water ratio only if compaction and curing remain adequate
SuperplasticiserLarger water reduction or high flowCompatibility, slump loss and overdosing matter
RetarderDelays setting; useful in hot weather or long placement operationsRetardation is not a guarantee of unchanged later strength
AcceleratorSpeeds setting and/or early strength development, depending on typeChloride-bearing accelerators can promote embedded-steel corrosion
Air entrainerStabilises many small distributed bubbles; improves freeze–thaw resistance and often workabilityEntrained air differs from large entrapped voids; strength usually falls at otherwise unchanged proportions
Viscosity modifierImproves cohesion and segregation resistanceDoes not remove the need for suitable grading

At a fixed water–binder ratio, improved flow does not imply weaker concrete. At fixed admixture dosage, adding water to restore slump changes the mix and can reduce strength and durability. Count water carried in a liquid admixture where relevant to the stated mix calculation.

2.5 Mineral admixtures and pozzolanic reaction

Past papers · CE 2020–2026 (14 papers): 1 question, 1 mark

AdditionMain characterRevision consequence
Fly ashPozzolanic; some high-calcium ashes also show cementitious actionOften slower early strength and lower heat; adequate curing is important
Silica fumeVery fine, highly reactive silicaPore refinement and improved ITZ; high surface area can increase water demand
MetakaolinReactive calcined clay, pozzolanicCan improve strength and reduce transport when properly proportioned
Ground granulated blast-furnace slag (GGBS)Latent hydraulicActivated in the cement system; do not describe it as only an inert filler
Limestone powderFiller/nucleation effects and possible chemical interactionNot equivalent to a reactive siliceous pozzolan

Mineral additions can reduce clinker demand and improve later-age properties; neither improvement nor a fixed replacement percentage is universal. In a blended mix distinguish cement mass from total cementitious mass. Longer moist curing may be required than for OPC concrete (Section 5.4).

Last-minute recall

  • C3SC_3S: earlier strength; C2SC_2S: later strength and lower heat.
  • C3AC_3A reacts rapidly and requires sulphate control.
  • C–S–H is the principal binding product; CH is calcium hydroxide.
  • Setting, hardening and drying are different processes.
  • More connected capillary pores usually mean easier ingress and lower durability.
  • A pozzolan reacts with CH; GGBS is latent hydraulic.
  • Water reducers can increase flow without increasing the water ratio.
  • OPC cement grade is a mortar-test grade, not a concrete grade.