Chapter 1

Steel as a construction material

Separate strength from stiffness and ductility. Steel grade chiefly sets a strength requirement; processing, composition and temperature determine how the material reaches and passes that strength.

1.1 Composition and processing

Past papers · CE 2020–2026 (14 papers): 1 question, 1 mark

Steel is an iron–carbon alloy with controlled alloying elements and impurities. Ordinary structural steels are predominantly low-carbon steels; a single carbon percentage does not describe all grades. IS 2062:2011 covers hot-rolled structural steel; IS 1786:2008 covers high-strength deformed reinforcement.

Change or constituentPrincipal effect to rememberQualification
More carbonUsually raises hardness, tensile strength and yield/0.2% proof stress; reduces ductility and weldabilityCompare broadly similar processing and microstructure
ManganeseStrengthening and deoxidation; combines with sulphurComposition limits depend on grade
SiliconDeoxidation and strengtheningNot a substitute for carbon in grade identification
Chromium, nickel, molybdenumCan improve hardenability, toughness or corrosion performanceEffects depend on the alloy and treatment
Excess sulphur/phosphorusCan impair ductility, toughness and fabrication behaviourDo not treat impurities as universally beneficial strength additions
Cold workingHigher yield strength/hardness, lower remaining ductility; residual stressElastic modulus changes little
Quenching followed by temperingCan combine increased strength with useful toughnessQuenching alone may produce a brittle condition
Thermomechanical treatment of reinforcing barsHarder outer region with a more ductile coreTMT describes processing, not a unique yield strength

Ferrite is relatively soft and ductile; cementite is hard and brittle; pearlite is a ferrite–cementite mixture. Increasing pearlite content in comparable plain-carbon steels generally increases strength. Full phase-diagram calculations are outside this CE topic.

1.2 Tensile response and proof stress

A mild-steel engineering tensile curve has an initial nearly linear region, yielding, strain hardening, an ultimate engineering stress and necking. Some high-strength/cold-worked steels have no distinct yield plateau; use the specified proof stress. Ultimate engineering stress uses the original area even after necking begins.

The elastic unloading line is approximately parallel to the initial slope. Its strain-axis intercept measures permanent strain. Percentage elongation after fracture uses the reassembled final gauge length; reduction of area uses the smallest fractured section. Resilience is elastic energy per unit volume; toughness is the total area under the stress–strain curve up to fracture. A stronger steel need not be tougher.

Engineering tension response and the construction of 0.2% proof stress; curves are schematic.Engineering tension response and the construction of 0.2% proof stress; curves are schematic.

1.3 Physical properties and service behaviour

For ordinary structural steel, the nominal material constants below follow IS 800:2007. Actual grade, thickness, temperature and product specification govern strength; do not infer strength from these physical constants.

QuantityRevision valueUse
Density ρs\rho_s7850 kg/m³Mass from volume
Young's modulus EsE_s2.0×1052.0\times10^5 MPaSmall elastic deformation
Poisson's ratio ν\nu0.30Elastic transverse contraction
Shear modulus GGAbout 0.769×1050.769\times10^5 MPaConsistent with isotropic elastic moduli
Thermal expansion coefficient αs\alpha_s12×10−612\times10^{-6} K−1^{-1}Free thermal movement

Fatigue is damage under repeated stress cycles and can occur below the static yield stress. Brittle fracture depends on toughness, temperature, flaws and constraint. Corrosion reduces section and can impair bond; adequate protection is needed even when a grade is described as corrosion-resistant. Fire reduces stiffness and strength: ambient-temperature constants are not fire-design values. Stress relaxation is stress reduction at maintained strain; creep is increasing strain at maintained stress.

Last-minute recall

  • Carbon generally increases strength but reduces ductility and weldability.
  • Strength grade does not determine elastic modulus.
  • Proof stress uses an offset parallel to the initial elastic slope.
  • At 0.2% proof stress, total strain includes the 0.002 permanent offset.
  • Engineering stress uses original area throughout the tensile test.
  • d2/162.2d^2/162.2 gives bar mass per metre only when dd is in mm.
  • Fatigue, brittle fracture and yielding are different failure mechanisms.

Revise offline: the whole Construction Materials and Management handbook as one PDF

51 pages · 2.2 MBFree to read online. Sign in to download the PDF.We save the handbook, version and request time in My downloads. Privacy policy