Chapter 9

Non-destructive testing

NDT detects discontinuities or changes in material response while keeping the component usable. Select a method by material, defect location and orientation, access and required resolution. A detected indication is not automatically a rejectable defect; acceptance needs a stated specification.

9.1 Method selection and operating principles

MethodPhysical indicationSuitable targetPrincipal limitation
Visual/opticalDirect surface appearanceAccessible cracks, corrosion, gross shapeLine of sight, illumination and resolution
Liquid penetrantCapillary entry, then developer draws out trapped liquidSurface-opening flaws in clean, nonporous materialCannot reveal a sealed internal flaw; porosity/contamination gives background
Magnetic particleFlux leakage attracts magnetic particlesSurface and near-surface cracks in ferromagnetic partsUnsuitable for nonferromagnetic materials; orientation matters
Eddy currentChange in induced currents and probe impedanceSurface/near-surface flaws in electrically conducting materialLift-off, conductivity and geometry changes also affect signal
UltrasonicEcho or transmitted-sound changeInternal discontinuities, thicknessCoupling, attenuation, coarse grain and reflector orientation
RadiographicX-ray/gamma-ray transmission contrastInternal density/thickness variations, porosity and inclusionsRadiation precautions; projection overlap; tight cracks may be missed

The broad method/material distinctions follow the ASNT method overview. Penetrant inspection proceeds through cleaning, drying, penetrant application and dwell, excess removal, developer application, inspection and post-cleaning. Removing too much penetrant from a crack can suppress its indication. See ASNT penetrant principles.

For magnetic-particle inspection, a crack cutting across magnetic flux produces a stronger indication than one parallel to it; use more than one magnetisation direction when flaw direction is unknown. Eddy-current inspection requires conductivity, not ferromagnetism. Austenitic stainless steel should not be assumed suitable for magnetic-particle testing merely because it is called steel.

Acoustic emission listens for transient elastic waves from active events under load; it does not simply image every dormant crack. Infrared thermography looks for altered thermal patterns; leak testing identifies a through-path using a pressure, bubble or tracer response. These are useful complements, not interchangeable substitutes for volumetric imaging.

9.2 Ultrasonic time of flight

A conventional contact ultrasonic probe uses a piezoelectric element to transmit and receive sound. Couplant reduces the air gap and improves transmission. An A-scan displays echo amplitude against travel time; a flaw echo before the back-wall echo corresponds to a shorter path, subject to the selected ray geometry. Pulse-echo can use one-sided access, while through-transmission typically needs transmitter and receiver on opposite sides.

If two successive back-wall echoes are separated by Δt\Delta t, plate thickness is cuΔt/2c_u\Delta t/2 for a normal beam. For one-way through-transmission time, omit the factor of two. Higher frequency shortens wavelength and can improve resolution, but generally increases attenuation and scattering. An echo requires suitable reflector orientation; lack of an echo alone does not prove absence of a flaw. See ASNT ultrasonic principles.

9.3 Radiographic attenuation and eddy-current depth

Radiography responds to the integrated attenuation along a ray. A void often transmits more radiation than surrounding solid; display brightness depends on the imaging convention. Planar cracks are easiest to reveal when their orientation gives a sufficient path-length contrast. Radiography generally provides less direct depth localisation than pulse-echo ultrasound from a known surface.

Increasing frequency, permeability or conductivity reduces the ideal skin depth. Probe lift-off and nonconductive coating thickness alter the coupling, so use appropriate calibration standards. The induced-current principle and conductivity dependence are described in ASNT electromagnetic testing.

Last-minute recall

  • Penetrant reveals surface-opening flaws in suitable nonporous material.
  • Magnetic particles require ferromagnetism; eddy currents require electrical conductivity.
  • Magnetic flux should cross the crack for strong leakage.
  • Pulse-echo time contains the outward and return paths.
  • Angle-beam path length is not the same as normal depth.
  • Radiography integrates along the ray and can miss unfavourably oriented tight cracks.
  • Higher ultrasonic frequency reduces wavelength but usually increases attenuation.
  • Higher eddy-current frequency reduces penetration depth.
  • A flaw indication needs a stated acceptance criterion before rejection.