Chapter 4

Highway materials and bituminous mixes

A pavement needs a stable subgrade, durable aggregates and a binder suited to its temperature and loading. Test names, reporting units and mass/volume bases are as important as numerical calculations.

4.1 Subgrade tests

Past papers · CE 2020–2026 (14 papers): 1 question, 2 marks

The California Bearing Ratio (CBR) is an empirical penetration-resistance index, not a modulus. Moisture content, density, soaking and surcharge affect the result. Design soaked CBR represents adverse moisture conditions; a four-day soaking period is the conventional test condition.

Correct an initially concave-up load–penetration curve by extending the tangent at its steep portion back to the penetration axis and using that intercept as corrected zero. Seating or alignment errors can create the concavity. Do not divide by 100 twice: a reported CBR of 6% enters an empirical CBR-number correlation as 6. The plate reaction modulus depends on loaded size and foundation conditions; it is not Young's modulus.

4.2 Aggregate tests

Past papers · CE 2020–2026 (14 papers): 2 questions, 3 marks

Property requiredTest and reported result
Resistance to crushingAggregate crushing value: fines as percentage of original sample mass
Resistance to impactAggregate impact value: percentage fines after standard impacts
Resistance to abrasion/wearLos Angeles abrasion: percentage mass loss; principally hardness/wear resistance
Resistance to weatheringSoundness: loss after salt-solution wetting/drying cycles
Good particle shapeFlakiness and elongation indices, percentage by mass
Binder adhesion in waterStripping value: percentage exposed aggregate surface after the prescribed treatment
Low absorption and adequate densityWater absorption and specific gravity
Surface frictionResistance to polishing; angular texture helps interlock and skid resistance

Lower crushing, impact and abrasion losses generally mean more resistant aggregate. Do not swap the impact and abrasion tests. Surface-course specification limits differ from base-course limits; a single acceptance percentage does not apply to every layer.

A flaky particle has thickness less than 0.6 times its mean sieve size; an elongated particle has length greater than 1.8 times that size. For a combined test after flaky particles are removed, track the mass basis explicitly: remaining-sample elongation percentage cannot simply be added to the original-sample flakiness percentage. On a common original basis, the combined percentage is 100(Mf+Me,remaining)/M0100(M_f+M_{e,\rm remaining})/M_0.

4.3 Bitumen tests and grading

Past papers · CE 2020–2026 (14 papers): 4 questions, 5 marks

TestMeaning and reporting unit
PenetrationConsistency; tenths of a millimetre; conventional condition 25°C, 100 g total load, 5 s
Ring-and-ball softening pointTemperature (°C) at a specified softening condition; bitumen has no single sharp melting point
DuctilityExtension before rupture, cm; conventional condition 27°C and 50 mm/min
Absolute/dynamic viscosityFlow resistance, Pa·s or poise; 11 poise =0.1=0.1 Pa·s
Kinematic viscosityDynamic viscosity/density, m²/s or cSt; 11 cSt =10−6=10^{-6} m²/s
Flash pointTemperature at momentary ignition of vapour under the test flame
Fire pointTemperature permitting sustained burning under the test conditions
SolubilitySoluble fraction (%): binder purity
Thin-film/rolling thin-film ovenShort-term ageing; report mass change and specified properties of the residue
Specific gravityDensity relative to water, dimensionless

Greater penetration means softer binder; a harder binder generally has higher softening point. Hot climates require resistance to softening and rutting; low temperatures require resistance to brittle cracking. Viscosity controls mixing and compaction temperatures. Conventional paving bitumen is viscosity graded (VG-10, VG-20, VG-30, VG-40); do not interpret these as penetration grades. Absolute viscosity at 60°C and kinematic viscosity at 135°C describe different properties. An oven test's heating duration is not its reported mass-loss unit.

4.4 Specific gravity and mix volumetrics

Past papers · CE 2020–2026 (14 papers): 4 questions, 8 marks

Use fractions by total mixture mass unless another basis is stated. Aggregate bulk, aggregate effective, maximum theoretical mix and compacted bulk mix specific gravities describe different volumes. Absorbed binder belongs within aggregate bulk pores and is excluded from effective binder filling intergranular voids.

4.5 Marshall design and desirable mix properties

Past papers · CE 2020–2026 (14 papers): 2 questions, 3 marks

A mix needs stability against shear deformation, fatigue resistance, durability, workable compaction, adequate flexibility, low permeability and skid resistance. Too little binder reduces cohesion and durability; too much binder promotes bleeding and instability. Too many air voids permit water/air ingress; too few leave inadequate room for densification and expansion.

Marshall stability is the peak load sustained at the prescribed test condition, conventionally 60°C; flow is deformation at peak load, reported in mm or units of 0.25 mm. The conventional loading rate is 50.8 mm/min. State the specified compaction effort and specimen correction when supplied; do not transfer criteria between mix specifications.

As binder content increases through a normal design rangeUsual trend
StabilityRises to a maximum, then falls
Bulk densityRises to a maximum, then falls
FlowGenerally increases
Air voidsDecrease
VFBIncreases
VMAOften decreases then increases; not necessarily monotonic

The traditional graphical optimum-binder exercise averages the contents at maximum stability, maximum density and target air voids (often 4%). Actual acceptance requires all specified stability, flow, VMA and VFB limits to pass; many procedures select binder at target air voids and then check the remaining limits. GATE 2025 (CE2 Q28) treats 3–5% air voids as the range used to arrive at the optimum binder content. This is not permission to ignore the mix specification.

Last-minute recall

  • CBR compares loads at equal penetration; confirm a larger 5 mm result by repeating.
  • Abrasion measures wear resistance; impact measures toughness; soundness measures weathering resistance.
  • Penetration is in 0.1 mm; ductility in cm; softening and flash points in °C.
  • Blend gravity is harmonic with mass fractions.
  • VMA is air plus effective binder, each on compacted-volume basis.
  • VFB uses VMA as its denominator.
  • Stability and density have peaks; Marshall flow generally increases with binder.