Chapter 4

Tool materials, wear and life

A useful cutting material must retain hardness at the cutting temperature and survive the loading pattern. Tool life is usable cutting time until a stated rejection criterion, not elapsed shift time. Match the life law to the tool, work, feed, depth and environment used in the test.

4.1 Cutting-tool material selection

Hardness alone is insufficient: hot hardness, wear resistance, chemical stability, toughness and thermal-shock resistance all matter. Compare like grades; coatings and edge preparation can change behaviour substantially.

Tool familyPrincipal advantageTypical use / limitation
Carbon tool steelLow cost; easy shapingLow-speed tools; loses useful hardness at lower temperature than HSS
High-speed steel (HSS)Tough and readily resharpened into complex shapesDrills, taps, broaches, form tools; lower speed capability than carbides
Cast cobalt-base alloyBetter hot hardness than ordinary tool steelWear-resistant cutting edges; less readily shaped than HSS
Cemented carbideHard carbide particles with metallic binder; useful hardness–toughness balanceGeneral turning/milling; more brittle than HSS; WC–Co is a common base
Coated carbideWear/chemical barrier on a supporting substrateCoatings such as TiN, TiCN and alumina extend usable conditions; substrate still matters
CermetTiC/TiCN-based hard phase with metal binderFinishing steels; edge wear resistance, but limited shock tolerance
Alumina / silicon-nitride-based ceramicHigh hot hardnessHigh-speed cutting under suitable conditions; avoid treating all ceramics as equally shock resistant
Cubic boron nitride (CBN/PCBN)Very high hardness and stability against ferrous workHardened steels and hard cast irons; expensive
Diamond / PCDExtreme hardness and abrasion resistanceNon-ferrous alloys, abrasive composites and non-metals; generally unsuitable for hot cutting of steels because of chemical wear

Traditional 18–4–1 HSS denotes approximately 18% tungsten, 4% chromium and 1% vanadium by mass; it is one grade family, not the composition of every HSS. Carbide binder improves toughness while excessive binder reduces hardness/wear resistance. Tool material choice must also consider interrupted versus continuous cutting. Supporting material-selection notes: common tool materials and advanced tool materials.

4.2 Wear, failure, machinability and cutting fluids

ObservationLocation / mechanismConsequence
Flank wearClearance face rubbing the new surface; abrasion and adhesionGrowing wear land, dimensional error, friction and poorer finish
Crater wearRake face under flowing chip; adhesion/diffusion at elevated temperatureWeakens edge and changes effective rake
Notch wearLocalised wear near depth-of-cut lineCan initiate fracture and damage finish
Edge chipping / fractureMechanical shock, brittle edge or excessive loadSudden failure rather than gradual wear
Thermal cracksRepeated heating/cooling, often across an interrupted-cut edgeCracks can develop even when mean temperature is acceptable
Plastic edge deformationHot strength insufficient for contact stressEdge loses its intended geometry

The usual flank-wear curve has rapid initial bedding-in, a relatively steady useful-wear stage and accelerated final wear. A specified wear-land width, crater limit, loss of tolerance/finish or failure can define life. Do not assume a numerical wear limit unless supplied.

Machinability may be judged by tool life, cutting force/power, surface finish or chip control. A ranking under one criterion need not match another. A machinability index based on cutting speed at equal specified life is 100Vtest/Vreference100V_{\rm test}/V_{\rm reference}; both speeds must use comparable test conditions.

Cutting fluids provide cooling, lubrication and chip flushing. Water-based emulsions emphasise cooling; oils provide stronger lubrication in suitable operations. Avoid abrupt cooling of a hot, thermally sensitive edge. Built-up edge is adhered work material; it is not the same thing as gradual tool wear. Coating and fluid selection do not remove the need for adequate edge strength.

Qualitative wear stages with a stated rejection limit; axes do not assign a universal wear criterion.Qualitative wear stages with a stated rejection limit; axes do not assign a universal wear criterion.

4.3 Taylor and extended tool-life laws

Past papers · ME 2020–2026 (10 papers): 1 question, 2 marks

Use a fixed rejection criterion. Here V,T,nV,T,n denote speed, cutting life and the life exponent in both laws. Taylor's exponent and constant are fitted parameters, not universal material constants. A log–log plot of speed against life has slope −n-n.

4.4 Parts per edge and changing cutting conditions

Past papers · ME 2020–2026 (10 papers): 1 question, 2 marks

Here TT is cutting life, tmt_m cutting time per part, nn the Taylor exponent and VV cutting speed in VTn=CTVT^n=C_T, with fitted constant CTC_T. A tool can spend considerable time travelling without cutting. Only the cutting-time contribution belongs in the usual Taylor life law. For drilled holes, raising rpm shortens the cutting time per hole when feed per revolution is held fixed.

For continuously varying speed, the same damage model gives ∫dt/T(V(t))=1\int dt/T(V(t))=1. With VTn=CTVT^n=C_T, this is ∫(V(t)/CT)1/ndt=1\int (V(t)/C_T)^{1/n}dt=1. Retain the same time units as those used for TT. This is not a claim that real wear is independent of thermal history.

Last-minute recall

  • Hot hardness and toughness are separate requirements.
  • HSS suits complex, resharpenable tools; carbide permits higher cutting speeds in suitable conditions.
  • CBN is useful for hard ferrous work; diamond is generally chosen for non-ferrous/abrasive work.
  • Flank wear is on the clearance face; crater wear is on the rake face.
  • The useful wear stage lies between initial rapid wear and final acceleration.
  • Taylor life is cutting time to a specified criterion.
  • CTC_T changes numerically if speed or time units change.
  • Convert drilled-hole counts to cutting time before finding nn.
  • Fractional parts per edge is an average, not a guaranteed complete-part count.
  • Linear damage accumulation needs an explicit modelling assumption.

Revise offline: the whole Machining and Machine Tools handbook as one PDF